Research paper
Experimental Characterization| Type | Label | Value | Material | Sample | Condition | Source |
|---|---|---|---|---|---|---|
| Layer Thickness | Al0.92Ga0.08As layer thickness | 133.2nm | — | |||
| Layer Thickness | GaAs layer thickness | 115.6nm | — | |||
| Stack Repeat Count | coating pair count | 38.5 | — | |||
| Cavity Birefringence Frequency Splitting | fast-slow axis splitting | 104kHz | — | |||
| Birefringence | Δnbiref | 0.00045 | — | |||
| Cavity Finesse | slow axis finesse | 129000 | — | |||
| Cavity Finesse | fast axis finesse | 128200 | — | |||
| Cavity Zero Crossing Temperature | CTE zero crossing | 297K | — | |||
| Beam Radius | plane mirror 1/e2 beam radius | 496um | — | |||
| Beam Radius | concave mirror 1/e2 beam radius | 687um | — | |||
| Coating Penetration Depth | lpen | 286nm | — | |||
| Free Spectral Range | cavity free spectral range | 312MHz | — |
| Type | Label | Value | Material | Sample | Condition | Source |
|---|---|---|---|---|---|---|
| Layer Thickness | Al0.92Ga0.08As layer thickness | 133.2nm | — | |||
| Layer Thickness | GaAs layer thickness | 115.6nm | — | |||
| Stack Repeat Count | coating pair count | 38.5 | — | |||
| Cavity Birefringence Frequency Splitting | fast-slow axis splitting | 104kHz | — | |||
| Birefringence | Δnbiref | 0.00045 | — | |||
| Cavity Finesse | slow axis finesse | 129000 | — | |||
| Cavity Finesse | fast axis finesse | 128200 | — | |||
| Cavity Zero Crossing Temperature | CTE zero crossing | 297K | — | |||
| Beam Radius | plane mirror 1/e2 beam radius | 496um | — | |||
| Beam Radius | concave mirror 1/e2 beam radius | 687um | — | |||
| Coating Penetration Depth | lpen | 286nm | — | |||
| Free Spectral Range | cavity free spectral range | 312MHz | — |
| Type | Label | Value | Material | Sample | Condition | Source |
|---|---|---|---|---|---|---|
| Layer Thickness | Al0.92Ga0.08As layer thickness | 133.2nm | — | |||
| Layer Thickness | GaAs layer thickness | 115.6nm | — | |||
| Stack Repeat Count | coating pair count | 38.5 | — | |||
| Cavity Birefringence Frequency Splitting | fast-slow axis splitting | 104kHz | — | |||
| Birefringence | Δnbiref | 0.00045 | — | |||
| Cavity Finesse | slow axis finesse | 129000 | — | |||
| Cavity Finesse | fast axis finesse | 128200 | — | |||
| Cavity Zero Crossing Temperature | CTE zero crossing | 297K | — | |||
| Beam Radius | plane mirror 1/e2 beam radius | 496um | — | |||
| Beam Radius | concave mirror 1/e2 beam radius | 687um | — | |||
| Coating Penetration Depth | lpen | 286nm | — | |||
| Free Spectral Range | cavity free spectral range | 312MHz | — |
| Type | Label | Value | Material | Sample | Condition | Source |
|---|---|---|---|---|---|---|
| Layer Thickness | Al0.92Ga0.08As layer thickness | 133.2nm | — | |||
| Layer Thickness | GaAs layer thickness | 115.6nm | — | |||
| Stack Repeat Count | coating pair count | 38.5 | — | |||
| Cavity Birefringence Frequency Splitting | fast-slow axis splitting | 104kHz | — | |||
| Birefringence | Δnbiref | 0.00045 | — | |||
| Cavity Finesse | slow axis finesse | 129000 | — | |||
| Cavity Finesse | fast axis finesse | 128200 | — | |||
| Cavity Zero Crossing Temperature | CTE zero crossing | 297K | — | |||
| Beam Radius | plane mirror 1/e2 beam radius | 496um | — | |||
| Beam Radius | concave mirror 1/e2 beam radius | 687um | — | |||
| Coating Penetration Depth | lpen | 286nm | — | |||
| Free Spectral Range | cavity free spectral range | 312MHz | — |